Glaze pinholes and bubbles (釉面针孔, yòumiàn zhēnkǒng) are among the most common fired-surface defects in porcelain. While firing is often blamed, the root cause frequently lies in the forming and glazing stages: trapped air, residual moisture, organic contamination, or incorrect slip properties create voids that punch through the molten glaze during firing. Understanding these forming-side causes is the first step to elimination.
What Are Pinholes and Bubbles?
A pinhole is a tiny crater on the fired glaze surface, formed when gas or vapour escapes through the molten glaze but the glaze does not fully heal before cooling. A bubble is a trapped gas pocket beneath or within the glaze that fails to escape. Both originate from gases—water vapour, air, or organic decomposition products—moving through the body-glaze system during firing.
The Forming-Side Causes
1. Mould Moisture Out of Range
Jiggering and slip-casting moulds must hold the correct moisture. Moulds that are too dry (below the ideal 5–6% water) absorb water too quickly, disrupting the body surface and producing pinholes. Moulds that are too wet (10–18% water) absorb too slowly, leaving a weak, water-logged surface that also generates defects.
2. Body Too Dry or Too Hot Before Glazing
If the body is over-dried or hot when glaze is applied, and the surface is not thoroughly wetted during washing, the glaze cannot be absorbed uniformly. Air is sealed beneath the glaze film and emerges as pinholes or bubbles during firing.
3. Body Too Wet When Glazed
Glazing a wet body and loading it into the kiln without drying forces a large volume of water vapour to escape during firing, punching pinholes through the glaze. If the temperature rises too rapidly, the escaping vapour can even cause blistering.
Maximum permissible body moisture before firing depends on the firing speed:
| Product Type | Maximum Body Moisture Before Firing |
|---|---|
| Tableware & sanitary ware (normal firing) | ≤ 2% |
| Wall & floor tiles (fast firing) | ≤ 1% |
| Fast-fired tile (very fast cycle) | ≤ 0.5% |
4. Incomplete Fettling and Organic Dust
If fettling is incomplete and organic dust or debris adheres to the body, it burns out during firing, leaving pinholes in the glaze above.
5. Glaze Slip Too Thin or Too Thick
An incorrectly proportioned glaze slip causes more than crazing. Over-thin or over-thick slips tend to trap gas at the body-glaze interface, leading to pinholes and bubbles.
6. Slip Casting Too Fast or Overheated Slip
Pouring slip too quickly leaves air pockets in the cast. Overheated slip can sour (ferment), losing water and trapping bubbles that are hard to release. Both produce pinholes after firing.
7. Carbon Pickup from Waste-Heat Drying or Aged Dust
Drying wet bodies on kiln waste heat for too long causes the body to absorb carbon, which burns out as gas during firing. Similarly, bodies left too long before firing accumulate organic dust; if not blown clean before loading, the dust volatilises and creates defects.
8. Glaze Layer Too Thin
An excessively thin glaze can be partially absorbed into the porous body, leaving the surface too sparse to heal over escaping gas—resulting in pinholes.
9. Poor Mould Design and Mould Dust
Moulds that do not vent properly trap gas in the body, which migrates to the surface during firing. Dust left on the mould surface volatilises during firing and also causes pinholes.
10. Poor Glazing Technique
Several glazing-line errors cause defects:
– Dust on the body that is not removed before glazing.
– The glaze line running too fast, so the glaze curtain seals air between body particles; this air breaks through as pinholes or stays as bubbles.
– Base glaze and face glaze applied too far apart, so the face glaze traps bubbles from the base coat.
11. Uneven Body Drying
This is one of the most insidious causes. Where a part of the body is not fully dry, it stays warmer and shrinks less, with larger inter-particle gaps. During glazing, water saturates this region quickly. As the water vaporises under body heat, it concentrates its escape at that spot—exactly while the glaze is setting. The result is a cluster of invisible micro-pores that become pinholes or bubbles after firing.
Table — Summary of Forming-Side Causes and Remedies
| # | Cause | Primary Remedy |
|---|---|---|
| 1 | Mould too dry or too wet | Hold mould moisture at 5–6%; avoid 10–18% wet range |
| 2 | Body too dry/hot, uneven wetting | Condition body temperature; wet surface thoroughly |
| 3 | Body too wet at glazing/firing | Respect moisture limits (2% / 1% / 0.5% by product) |
| 4 | Organic dust, incomplete fettling | Complete fettling; clean body before glazing |
| 5 | Glaze slip wrong viscosity | Calibrate slip density and viscosity |
| 6 | Fast pouring, sour slip | Pour gently; control slip temperature and age |
| 7 | Carbon pickup, aged dust | Limit waste-heat drying; blow bodies clean |
| 8 | Glaze too thin | Increase glaze thickness to specification |
| 9 | Poor mould venting, mould dust | Redesign vents; clean moulds before use |
| 10 | Glazing-line errors | Clean bodies, slow glaze line, sequence glazes closely |
| 11 | Uneven body drying | Ensure uniform drying before glazing |
Frequently Asked Questions
Are glaze pinholes always caused by firing?
No. Many pinholes originate in forming and glazing—trapped air, residual moisture, and organic dust create gas that escapes through the glaze during firing. Fix the forming-side causes before adjusting the kiln profile.
What is the correct mould moisture for slip casting?
Moulds should hold about 5–6% moisture. Below that they absorb too fast; above 10% they absorb too slowly. Both extremes promote pinholes.
How dry must the body be before firing?
It depends on firing speed. Tableware and sanitary ware should be below 2% moisture; wall and floor tiles below 1%; very fast-fired tiles below 0.5%. Faster firing demands drier bodies because water vapour has less time to escape gently.
Why does uneven drying cause invisible defects that only appear after firing?
A damp zone has larger particle gaps. Water from glazing concentrates there and vaporises during drying, punching micro-pores through the setting glaze. These pores are nearly invisible on the raw glaze but open into pinholes during firing.
Related Reading
Pair this with Ceramic Glaze Dullness: Origins of Matte Surfaces and Their Prevention, Ceramic Firing Stages: Temperature Zones and Atmosphere Control, and Ceramic Cracking Defects: Seven Types and Their Prevention.
For glaze-consulting or commissions on high-quality Jingdezhen porcelain, visit our shop or email our studio.