Six properties decide how a clay behaves in the workshop: plasticity (可塑性, kěsùxìng), binding power (结合性, jiéhéxìng), thixotropy (触变性, chùbiànxìng), drying behaviour (干燥性能, gānzào xìngnéng), sintering (烧结性, shāojiéxìng) and refractoriness (耐火度, nàihuǒdù). Each can be measured, and each has a working range. Knowing the numbers behind them turns a vague “this clay feels wrong” into a diagnosis.
1. Plasticity — The Base Property
Plasticity is the ability of a wetted clay mass to be shaped under an external force and to hold that shape once the force is removed. Four factors govern it.
| Factor | Effect on Plasticity |
|---|---|
| Clay mineral structure | Layered (sheet) structures raise plasticity; the plates slide over one another |
| Degree of dispersion | Finer particles mean greater surface area, more contact points, higher plasticity |
| Particle shape | Flake-like particles slide and bond better than angular ones |
| Liquid chemistry | Only hydroxyl-bearing liquids such as water form a soft mass; hydrocarbons such as petrol or kerosene will not |
Plasticity peaks when the clay is easy to form yet does not stick to the hands. That condition is called the standard working mass (标准工作泥团), and the water content at that point is the plastic water content.
Table — Plastic Water Content by Clay Grade
| Clay Grade | Plastic Water Content |
|---|---|
| Highly plastic clay | 28–48% |
| Medium plasticity | 20–28% |
| Low plasticity | 15–20% |
2. Binding Power
Binding power is the ability of clay to combine with non-plastic (lean) materials to form a workable mass with adequate dry strength. Strongly plastic clays are usually strong binders, but the two properties are distinct and measured separately. The standard test mixes the clay with standard sand of fixed grading: 70% between 0.25 and 0.15 mm, 30% between 0.15 and 0.09 mm. The more sand a clay can absorb before the mass falls apart, the stronger its binding power.
3. Thixotropy and the Thickening Coefficient
Thixotropy is the property by which a slip loses viscosity when stirred or vibrated and slowly regains it at rest. Some thixotropy is useful; too much and the slip will not flow through pipes.
It is expressed as the thickening coefficient (稠化度): the ratio of the time needed for 100 ml of slip to flow from an Engler viscometer after standing 30 minutes, to the time needed after standing only 30 seconds, measured at the same temperature.
| Product | Target Thickening Coefficient |
|---|---|
| Fine porcelain slip (细瓷) | 1.8–2.2 |
| Fine earthenware (精陶) | 1.6–2.6 |
4. Drying Behaviour
Three measurements matter: drying shrinkage, dried porosity and dry strength. As water leaves, particles draw together and the body shrinks; the space left between particles becomes porosity. Dry strength directly sets the breakage rate during demoulding, transport, glazing, fettling and kiln loading. Mechanised and automated forming lines demand higher dry strength than hand work because the body is handled by machinery rather than by eye.
5. Sintering and Refractoriness
Sintering behaviour is tracked through firing shrinkage: during firing the body undergoes a series of physical and chemical changes and contracts in length or volume. Refractoriness is the temperature at which the body begins to soften and deform; a clay that is highly refractory widens the firing window but may need more flux to vitrify.
Table — Summary of the Six Properties
| Property | Measured By | Why It Matters |
|---|---|---|
| Plasticity | Plastic water content | Forming without cracking or collapsing |
| Binding power | Standard-sand addition test | Body strength with lean additions |
| Thixotropy | Thickening coefficient | Slip pumping, casting, glaze suspension |
| Drying behaviour | Shrinkage, porosity, dry strength | Losses at demoulding, transport, glazing |
| Sintering | Firing shrinkage | Dimensional control, deformation risk |
| Refractoriness | Softening temperature | Firing range and flux requirement |
Frequently Asked Questions
Why does my clay crumble instead of forming a soft mass?
Plasticity depends on the liquid as well as the clay. Only hydroxyl-bearing liquids such as water plasticise clay; a hydrocarbon such as kerosene will not. If water content is right and the clay still crumbles, the clay is probably low-plasticity (15–20% plastic water) and needs a plasticiser or ageing.
What is a good thickening coefficient for porcelain slip?
For fine porcelain, keep it between 1.8 and 2.2. Below that the slip may settle and separate; above it, flow in pipes and casting rate both suffer.
How do I test binding power myself?
Add standard sand in increasing proportions to a fixed clay sample and note the point at which the mass stops forming a coherent, handleable body. That sand fraction is a practical index of binding power.
Why does dry strength matter more on automated lines?
Machines cannot feel a weak rim. Handlers compensate by eye and hand; robots and take-off devices do not, so bodies with low dry strength fail far more often during demoulding, glazing and kiln loading.
Related Reading
See also Ceramic Slurry Iron Removal: Magnetic Separation and Process Control, Ceramic Drying Dynamics: Heat Transfer and Diffusion and Ceramic Firing Stages and Atmosphere Control.
Our studio selects and ages its clay bodies against these six properties. Browse finished work in the shop or email us about commissions.