Slip casting (注浆成型, zhùjiāng chéngxíng) is the backbone of sanitary ware, tableware and complex hollow-formed porcelain. A good cast depends not only on the slip and the mould, but on a disciplined sequence of preparation, pouring, draining and finishing. Below is the complete workflow, from mould inspection to final handling, with the critical parameters that decide success or defect.
1. Mould Preparation and Cleaning
New plaster moulds must be inspected to standard. Any grease or damaged spots on the inner surface must be removed. New mould moisture typically runs 6–8%; complex, small or thin-walled wares can tolerate higher moisture, while large flat wares need lower—never below 4%. Moulds are dried at a controlled room temperature of 28–35 °C to prevent uneven drying and distortion. Before use, dust and debris are cleaned off so the mould halves seal tightly and no slip leaks, and so the cast adheres correctly without contamination.
2. Mould Brushing (擦模)
Brushing the mould surface with water controls how the cast releases. In cold weather, clear water is used so the body can shrink freely in the mould without cracking. For new moulds, dry moulds, or large flat products such as tanks, troughs, the rim of a pedestal pan, or the concave side of a basin, mixed water (muddy water) is applied to increase the mould’s attraction to the slip.
Brushing force follows the age of the mould:
| Mould Condition | Brushing Force | Reason |
|---|---|---|
| New / dry mould | Firm | Open the pores to raise slip attraction |
| Mid-life mould | Medium to light | Pores already open; heavy brushing hinders release |
| Late-life / wet mould | Very light | Wipe with water only; heavy brushing causes cracking |
Focus areas include large flat surfaces (pedestal pan bodies, tank faces—must be even with no missed spots), convex/concave corners (firm but not excessive), the concave side of double-sided casting, and rim/cover parts. The upper opening of squat pans, tanks and pedestal bodies needs firm, even brushing to prevent premature release.
3. Assembly
Treated mould halves that are used in combination are aligned, clamped firmly, and the slip-drain hole plugged. Handle gently to avoid chipping the sealing edges.
4. Vent the Slip Line
Drain old slip and bleed air from the system before casting, so the first pour is clean and bubble-free.
5. Pouring
Fill the mould gently. A violent “slip shock” causes spots and ring marks on the cast. The slip should flow in smoothly and fill without splashing.
6. Determine Drain Time
Use a test casting cup to find the correct dwell (drain) time, so the wall reaches the required thickness before the surplus slip is poured out.
7. Draining (Draining the Slip)
Open the air vent before draining to avoid a suction effect that can distort the soft cast. Three drain methods are common:
- Gravity return—slope the pipe so surplus slip flows back to the tank by natural pressure.
- Slip-pump return—a pump draws surplus slip back through the return pipe; pipe leaks reduce effectiveness.
- Vacuum return—a vacuum pump creates negative pressure in the lower filling line to draw slip back.
8. Curing (巩固期)
After draining, the cast must stiffen in the mould. Too early and it collapses on release; too late and it shrinks against the mould and cracks where restrained. As a rule, curing lasts about half the casting (dwell) time.
9. Demoulding
Demould when the body moisture is roughly 19–20%. Soft casts that release without deforming require skilled handling.
10. Repair
After release, small cracks are repaired with slip and clay pegs (泥钉).
11. Assembly (修粘)
Attach the parts that belong together—pipes, rims, bases, lugs. Sanitary-ware bodies are assembled at 15–17% moisture. Attachments should be 2–3% drier than the main body, because parts shrink faster; matching moisture prevents uneven shrinkage and cracking.
12–15. Cutting and Holes
- Open holes only when the body is firm enough: too soft and it deforms, too hard and it risks later cracking.
- Choose the correct hole position and angle for the product model.
- Use properly designed and sharpened knives.
- Cut without tearing the surface—tearing creates weak points and surface defects.
16. Drying Speed
Control the drying rate. Once the body falls below its critical moisture, shrinkage is minimal and the body can be dried quickly without cracking. Before that point, slow, even drying is essential.
17–20. Handling and Housekeeping
- Keep the working area clean to avoid contaminating the soft body.
- Move large bodies with correct posture and technique to avoid stress cracks.
- Finish fettling while the surface is still soft, before a hard skin forms—this minimises harmful dust.
- After holidays or long breaks, recondition over-aged slip and dried moulds before resuming production.
Table — Critical Moisture and Temperature Parameters
| Stage | Parameter | Value |
|---|---|---|
| New mould moisture | Standard / minimum | 6–8% / ≥ 4% |
| Mould drying temperature | Room | 28–35 °C |
| Curing time | Relative to casting time | ≈ ½ of dwell time |
| Demoulding moisture | Body | 19–20% |
| Assembly moisture | Sanitary-ware body | 15–17% |
| Attachment moisture | Relative to main body | 2–3% drier |
Frequently Asked Questions
How moist should a new plaster mould be?
New moulds typically hold 6–8% moisture, never below 4%. Complex thin-walled wares can use slightly higher moisture; large flat wares need lower.
Why is brushing the mould so important?
Brushing controls the mould’s slip attraction and release. Clear water lets the body shrink freely (cold weather); mixed water increases attraction for new or dry moulds. Brushing force must match mould age—firm for new moulds, very light for late-life or wet moulds.
How long should the cast cure before demoulding?
About half the casting (dwell) time. Too early and the body collapses; too late and it shrinks against the mould and cracks.
At what moisture do you demould and assemble?
Demould at roughly 19–20% moisture. Assemble sanitary-ware bodies at 15–17%, with attachments 2–3% drier to balance shrinkage.
Why must the air vent be opened before draining?
Without venting, draining creates suction that can distort the soft, uncured cast. Always open the vent first.